K.27 · Material · 12 min read

Corrosion-Resistant MIM Materials 316L, 304L, 17-4 PH, titanium and cobalt-chromium with sourced data — and why the alloy alone does not secure corrosion resistance.

In metal injection moulding, corrosion resistance is not a pure material property. It is the result of alloy, sintered density, surface condition and post-treatment. A MIM part in 316L with insufficient sintered density is less corrosion resistant than a wrought part in the same alloy, because open residual porosity offers attack area and promotes crevice corrosion.

That is why every figure on this page is accompanied by the process condition under which it applies.

Property data

All values are supplier data from datasheets declaring conformity with MPIF Standard 35 or ASTM B883, or normative minimum values where those are freely available. Where minimum and typical values differ, both are given.

Material Condition Rm Rp0.2 A Density Hardness
MIM 316L as-sintered, minimum 450 MPa 140 MPa 40 % — —
MIM 316L as-sintered, typical 520 MPa 175 MPa 50 % 7.6 g/cm³ 67 HRB
MIM 304L as-sintered, supplier range 450 – 630 MPa 160 – 180 MPa 25 – 50 % 7.5 – 7.75 g/cm³ up to 100 HRB
MIM 17-4 PH as-sintered, minimum 790 MPa 650 MPa 4 % — 27 HRC
MIM 17-4 PH as-sintered, typical 900 MPa 730 MPa 6 % 7.5 – 7.66 g/cm³ 27 HRC
MIM Ti-6Al-4V ASTM F2885 Type 2, as-sintered 780 MPa 680 MPa 10 % 4.20 g/cm³ up to 30 HRC
MIM Ti-6Al-4V ASTM F2885 Type 1, densified 900 MPa 830 MPa 10 % close to 4.43 g/cm³ —
MIM CoCrMo as-sintered, supplier data 992 MPa 551 MPa 30 % 8.3 g/cm³ 25 HRC

Young's modulus for the stainless grades is around 190 GPa. The spread on MIM 304L is real and not an imprecision of this presentation: supplier figures differ considerably because 304L is not listed in MPIF Standard 35. Anyone specifying 304L should fix the property values supplier by supplier.

The figure that appears on no datasheet line Sintered density decides corrosion behaviour more than the last decimal of tensile strength. MPIF Standard 35 sets a minimum density for each MIM material; EPMA gives above 97 percent of theoretical density as the usual figure, and our series parts sit between 95 and 98 percent depending on material. Below that mark porosity becomes open and therefore corrosion-relevant. The density requirement belongs in the specification, not just the material name.

Selection by application

Requirement First choice Second choice Note
Moisture, perspiration, skin contact MIM 316L MIM Ti-6Al-4V 316L passivated, titanium resistant without post-treatment
Corrosion resistant and strong MIM 17-4 PH — considerably stronger than 316L, but less resistant to chlorides
Surgical instruments MIM 316L, MIM Ti-6Al-4V MIM CoCrMo implant suitability requires separate validation, see below
Chloride-bearing media MIM 316L at elevated density MIM Ti-6Al-4V molybdenum content and residual porosity decide jointly here
Low weight with resistance MIM Ti-6Al-4V — 4.2 g/cm³ against 7.6 g/cm³ for 316L

The four points that decide the outcome

Sintered density and open porosity

Closed porosity inside the part matters little for corrosion. Open porosity connected to the surface matters a great deal: it acts as a crevice in which medium collects and the passive layer breaks down locally. In sintered materials the transition from open to closed porosity lies around 92 to 95 percent of theoretical density. That is the reason for the density requirement.

Passivation

MIM 316L is passivated like any other austenitic stainless steel. The difference lies in the preparation: residual binder and carbon from debinding must be removed, otherwise no uniform passive layer forms. Passivation therefore belongs in the process agreement, not in the assumption.

Carbon and oxygen content

For titanium this is the critical point. ASTM F2885 limits oxygen to 0.20 percent and carbon to 0.08 percent. Both are picked up during debinding and sintering if the process is not set up for it. Exceedances embrittle the part without showing immediately in tensile strength — elongation falls first. The analysis belongs in the first article report.

Surface roughness

EPMA gives roughly Ra 0.8 µm for the as-sintered condition. For applications with a cleaning requirement or skin contact that is usually sufficient; for sealing faces and instrument geometries the part is polished or electropolished. Electropolishing additionally improves corrosion resistance because it removes the deformed and contaminated surface layer and enriches the surface in chromium. It does, however, expose near-surface pores — at low sintered density the result can therefore be worse than before treatment.

On biocompatibility Material conformity to ASTM F2885, F2886 or F2989 does not mean implant suitability. It is a material specification, not a product release. Suitability for a specific medical device follows from cleaning validation, sterilisability, surface condition, traceability and the regulatory route — not from the material number.

What belongs in the specification

  1. Material with standard, not just a short name
  2. Condition: as-sintered, heat treated, densified
  3. Minimum density as a percentage of theoretical density or in g/cm³
  4. Surface condition: as-sintered, blasted, polished, passivated, electropolished
  5. For titanium, additionally the permissible oxygen and carbon contents
  6. Measurement method for density, usually Archimedes or metallographic section

Our approach

We specify density and surface condition alongside the alloy, because the material name alone does not carry the requirement. For applications with a corrosion requirement we supply density and passivation evidence as part of the first article inspection, regardless of which plant produces the part.

Further reading

Questions about the topic of this article?

Our engineering and purchasing teams are available for technical enquiries — without obligation, without a form funnel.